| 性能項目 | 試驗條件[狀態] | 測試方法 | 測試數據 | 數據單位 | |
| 基本性能 | 熔體流動速率 | --- | ASTM D-1238 | 3 | g/10 min |
| 物理性能 | 吸收率 | 23°C,60%RH | ASTM D-570 | 0.36 | % |
| 填充材料含有率 | --- | --- | Super | % | |
| 比重 | --- | ASTM D-792 | 1.29 | --- | |
| 成型收縮率 | t3mm,直徑100mm | --- | 1.2 | % | |
| 機械性能 | 拉伸強度 | 23℃ | ASTM D-638 | 240 | kgf/cm2 |
| 伸縮率 | 23℃ | ASTM D-638 | >300 | % | |
| 彎曲強度 | 23℃ | ASTM D-790 | 260 | kgf/cm2 | |
| 曲折彈性率 | 23℃ | ASTM D-790 | 0.66 | ×104kgf/cm2 | |
| IZOD沖擊強度 | Notch t3.2mm | ASTM D-256 | >100 | kgf.cm/cm | |
| 拉伸沖擊強度 | t3.2mm S type | ASTM D-1822 | >=300 | kgf.cm/cm2 | |
| 洛氏硬度 | M scale | ASTM D-785 | M64 | --- | |
| 電氣性能 | 表面電阻率 | --- | ASTM D-257 | 1×1016 | Ω |
| 體積電阻率 | --- | ASTM D-257 | 1×1014 | Ω.cm | |
| 熱 性 能 | 燃燒性 | t0.8mm | UL 94 | HB | --- |
| 熔點 | 10C°/min | DSC Method | 165 | ℃ | |
| 熱變形溫度 | 4.6kgf/cm2 | ASTM D-648 | 125 | ℃ | |
| 熱變形溫度 | ×10-5cm/cm/℃ | ASTM D-648 | 70 | ℃ | |
| 線膨脹系數 | 20C°-80C° | ASTM D-696 | 13 | ×10-5cm/cm/℃ | |